Cr 20.5-24.0, Mn 4.0-7.0, Ni 9.5-12.0, Si 0.90, N 0.10-0.30,
C 0.05, P 0.03, S 0.03, Cu 0.75, Mo 1.5-3.0, V 0.10-0.30
High Performance Alloys stocks and produces this grade in the following forms: Weld Wire Request quote on this grade.
AWS 5.9 Class ER209 / ASME SFA 5.9 Class ER209
ER209 / UNS S20980
C | Cr | Ni | Mo | Mn | Si | P | S | N | Cu | V |
0.05 | 20.5 - 24.0 | 9.5 - 12.0 | 1.5 - 3.0 | 4.0 - 7.0 | 0.90 | 0.03 | 0.03 | 0.10 - 0.30 | 0.75 | 0.10 - 0.30 |
TYPICAL MECHANICAL PROPERTIES:
TENSILE STRENGTH | 101,500 PSI |
YIELD STRENGTH | 62,900 PSI |
ELONGATION MIN. | 36% |
IMPACT STRENGTH | 54.2 FT-LBS -4ºF |
MIG 25 lbs. spool 0.030” Dia, 0.035” Dia, 0.045” Dia, 0.062” Dia
TIG 36” 10lbs. tubes 0.062” Dia, 0.078” Dia, 0.093” Dia, 0.125” Dia, 0.187” Dia
TYPICAL WELDING PARAMETERS FOR ER209 (NITRONIC® 50W) WIRE:
WIRE DIA. | AMPERAGE | VOLTAGE | WIRE SPEED IN./MIN. | JOINT THICKNESS INCH | SHIELDING GAS |
0.030" 0.035" | 70 - 90 | 18 - 24 17 - 20 | 150 - 200 | 0.050 - 0.187 | 90He/7.5Ar/2.5Co2 69Ar/30He/1Co2 |
0.045” | 75 - 160 | 19 - 22 18 - 22 | 175 - 225 | 0.125 - 0.750 | 75Ar/25He 90He/7.5Ar/2.5Co2 69Ar/30He/1Co2 |
ALL PARAMETERS DIRECT CURRENT REVERSED POLARITY
GTAW Parameters same as 300 series stainless steels.
The gas tungsten arc, plasma arc, and electron beam processes are not suggested for direct application of this filler metal on mild steel.
The weld deposit has little or no ferrite. Care must be taken to avoid hot cracks. This is accomplished by low heat input and making “convex” bead profiles. Excessive weaving may also cause surface (hot short) cracks.
NITRONIC® Registered trade name of AK Steel